DIN 17441/EN 10088-2
Cold-rolled, surface finishes: 2R (IIId), 2B (IIIc), tolerances acc. to DIN 59382.
Hot rolled, surface finishes: 1D (IIa), 2D (IIIb), 2B (IIIc), tolerances acc. to EN 10029-81.
For 2B (IIIc) surface tolerances acc. to DIN 59382.
Chemical composition in % by weight
Steel grade
S (max)
Si (max)
Mn (max)
P (max)
S (max)
Cr
Mo
Ni
Others
X6CrNiTi 18-10 1.4541
0.08
1.0
2.0
0.045
0.015
17.0-19.0
9.0-11.0
Ti 5C-0.7
X6CrNiMoTi 17-12-2 1.4571
0.08
1.0
2.0
0.045
0.015
16.5-18.5
2.0-2.5
10.5-13.5
Ti 5C-0.7
X6Cr 17 1.4016
0.8
1.0
1.0
0.04
0.015
16.0-18.0
X2CrNiCrMo 17-13-2
0.07
1.0
2.0
0.045
0.015
16.5-18.5
2.0-2.5
10.0-13.0
N (max) 0.11
X15CrNiSi 20-12 1.4828
0.1
1.5-2.5
0.7
0.03
0.015
19.0-22.0
11.0-13.0
XINiCrMoCuN 25-20-5 1.4539
0.02
0.7
2.0
0.03
0.01
19.0-21.0
4.0-5.0
24.0-26.0
Cu 1.2-2.0N 0.15 Ti 0.5-0.9
Equivalent Standards
GOST
DIN
W.-Nr.
ASTM AISI
12X17
X6Cr17
1.4016
430
08X18H10
X5CrNi18-10
1.4301
304
03X17H14M3
X2CrNiMo17 132
1.4404
316L
03HN28MDT
X1NiCrCuMo25 205
1.4539
N08904
08X18H10T
X6CrNiTi18 10
1.4541
321
10X17H13M2T
X6CrNiMoTi17 122
1.4571
316Ti
GOST = gosudarstvennyj standard (Russia).
DIN = Deutsches Institut für Normung (German standards).
W.-Nr. = material number.
AISI = American Iron & Steel Institute.
ASTM = American Society for Testing and Materials.
Chemical composition of equivalent steel grades may vary. It depends on the insufficiency of different alloying elements in some countries. However, the differences in contents of such elements, as C, Cr, Ni, Cr, Mn, Mo and Ti are too small to have an effect on the structure and properties of equivalent materials.